Quick answer: laser welding heat input is Q = P / v, where P is laser power in watts and v is welding speed in mm/s. The result is expressed in J/mm. For 0.5–3 mm stainless and carbon steel, a well-tuned fiber laser weld sits between 8 and 45 J/mm — roughly one tenth of an equivalent TIG weld. Below 6 J/mm you get lack of fusion; above 80 J/mm thin sheet starts to bow.
1. The formula and what each term actually means
Q (J/mm) = P (W) ÷ v (mm/s). Power is measured at the workpiece, not at the source: a 2 kW source with 88% delivery efficiency puts 1,760 W into the part. Speed is the actual travel speed of the stage or robot, not the commanded feed rate. When either number is wrong by 10%, heat input is wrong by 10% — and so is your weld bead width.
Because the relationship is inverse, doubling speed halves heat input but also halves penetration depth. That single trade-off is why heat input charts and penetration charts are the same chart read in two directions.
2. Measured heat input by thickness
| Material | Thickness | Power (W) | Speed (mm/s) | Heat input (J/mm) | Typical result |
|---|---|---|---|---|---|
| 304 stainless | 0.5 mm | 500 | 60 | 8.3 | Conduction mode, no discolouration |
| 304 stainless | 1.0 mm | 1,000 | 50 | 20 | Full penetration, 0.9 mm bead |
| 304 stainless | 2.0 mm | 2,000 | 45 | 44 | Keyhole start, slight undercut |
| Q235 carbon steel | 3.0 mm | 3,000 | 40 | 75 | Keyhole, 3.0 mm penetration |
| Q235 carbon steel | 6.0 mm | 6,000 | 30 | 200 | Deep keyhole, needs fixture clamping |
Read the first column down and the pattern is obvious: every doubling of thickness costs a little more than double the heat input, because conduction losses grow with the thermal mass behind the weld.
3. Why J/mm matters more than watts
Two machines can both claim “2 kW” and produce completely different parts. At 20 mm/s the 2 kW machine delivers 100 J/mm and bows a 1 mm panel. At 80 mm/s the same machine delivers 25 J/mm and leaves the panel flat. Buyers who compare kilowatts are comparing the wrong number.
Heat input also drives three downstream costs: post-weld straightening, heat tint removal, and fixture wear. A 30% reduction in J/mm typically removes one straightening operation from a 1.5 mm stainless assembly.
4. Reading the defects back to the number
| Symptom | Heat input | First parameter to change |
|---|---|---|
| Lack of fusion at the root | Too low (< 6 J/mm) | Reduce speed 15%, keep power |
| Spatter on the top bead | Too high at the surface | Defocus +1 mm, raise speed |
| Undercut on both sides | Too high | Lower power 10%, add wobble |
| Blow-through on thin sheet | Far too high | Switch to pulsed mode, 30% duty |
| Grey/blue oxidation halo | Marginal | Increase shielding gas, not power |
5. How to hold heat input constant across a batch
Log P and v per part, not per shift. Drift hides in averages.
Measure power at the workpiece with a calorimeter once a month; delivery fibre degradation shows up as falling Q long before it shows as a bad weld.
Lock speed in the program and adjust power only — operators can feel a speed change, they cannot feel a 3% power change.
Keep a J/mm window per part number in the work instruction, the same way you keep a torque spec.
Frequently asked questions
Is laser welding heat input the same as arc welding heat input?
The formula is identical, Q = P/v, but the efficiency term differs. Arc processes lose 20–40% of the input to the arc and spatter; fiber laser delivery loses 8–15%. That is why a 20 J/mm laser weld and a 20 J/mm TIG weld do not produce the same heat-affected zone — the laser puts more of its energy where you aimed it.
What heat input do I need for 1 mm stainless?
18–25 J/mm for full penetration without distortion. On a 1 kW source that is 40–55 mm/s. Go below 15 J/mm and the root becomes intermittent; above 30 J/mm the part needs clamping or a copper backing bar.
Does wobble welding change the calculation?
Yes. Wobble spreads the same energy over a wider track, so effective heat input per unit area drops while Q per unit length stays the same. Use Q for distortion prediction and energy density (W/cm²) for penetration prediction — they move in opposite directions when you change amplitude.
Can I exceed 200 J/mm on thick plate?
You can, and on 8 mm and above you often must. The limit is not the number itself but the fixture: above roughly 150 J/mm, thermal expansion during the pass exceeds what a standard clamp can hold, and the part moves while it is being welded.
Related reading
Intouchray has manufactured industrial fibre laser cutting, welding, cleaning and cladding machines in Dongguan, Guangdong, China since 2001, with additional bases in Wuhan and Korea. Minimum order is one machine, built to order.