# Wobble Welding: Amplitude, Frequency and Gap Bridging Limits

[Home](https://www.intouchray.com) - [Technical Support](https://www.intouchray.com/category/technical-support/) - Wobble Welding: Amplitude, Frequency and Gap Bridging Limits

**Quick answer:** a static beam bridges about 0.1 mm of gap. Wobble at 1.0 mm amplitude bridges 0.4 mm, and at 1.5 mm amplitude it bridges 0.6 mm — at the cost of 20–35% of penetration. Amplitude is a fit-up allowance, not a quality improvement; use the smallest value that survives your worst joint.

## 1. Gap bridging by amplitude

| Amplitude | Frequency | Max gap (1 mm sheet) | Penetration loss |
| --------- | --------- | -------------------- | ---------------- |
| 0 (static) | — | 0.10 mm | 0% |
| 0.4 mm | 100 Hz | 0.20 mm | 5% |
| 1.0 mm | 150 Hz | 0.40 mm | 18% |
| 1.5 mm | 200 Hz | 0.60 mm | 32% |
| 2.0 mm | 250 Hz | 0.75 mm | 45% |

Frequency matters less than amplitude for bridging, but it matters for the bead surface. Below 50 Hz the oscillation leaves visible scallops; above 200 Hz the surface closes and looks like a static weld.

## 2. Why wobble costs penetration

The beam spends less time at any single point. At 1.5 mm amplitude and 150 Hz the spot sweeps 450 mm/s sideways on top of the travel speed, so dwell time per point drops by more than half. You can recover some of it with 15–20% more power, but not all of it — the keyhole does not have time to stabilise.

## 3. Settings by joint

| Joint | Amplitude | Frequency | Reason |
| ----- | --------- | --------- | ------ |
| Butt, laser-cut, tight | 0.3 mm | 150 Hz | Only for appearance |
| Butt, sheared, 0.2 mm gap | 0.8 mm | 150 Hz | Bridges shear tolerance |
| Lap, 0.5 mm gap | 1.2 mm | 180 Hz | Widens the fusion zone |
| Fillet, galvanized | 1.0 mm | 250 Hz | Vents zinc vapour |

## Frequently asked questions

### Does wobble improve weld appearance?

It widens the bead and softens the toe angle, which is good for fatigue. It does not remove spatter and it does not fix a bad fit-up beyond the bridging limit.

### Can I wobble on 0.5 mm sheet?

Marginally. Amplitude approaching sheet thickness causes burn-through at the oscillation extremes. Keep amplitude below 60% of thickness on anything under 1 mm.

### Is twin-spot better than wobble?

For very wide seams, yes — twin-spot keeps two stable keyholes instead of one moving one. For gap bridging, wobble is cheaper and retrofittable.

## Related reading

- [Penetration depth per kW](https://www.intouchray.com/laser-welding-penetration-depth-mm-per-kw/)

- [Galvanized steel laser welding](https://www.intouchray.com/galvanized-steel-laser-welding-zinc-porosity-parameters/)