Quick answer: on carbon steel at 30 mm/s, penetration runs close to 1 mm per kW from 1 kW to 6 kW. Above 6 kW the curve flattens because plasma absorption in the keyhole caps how much energy reaches the bottom. If you need 10 mm, plan for 12 kW plus helium, not 10 kW.
2. Measured penetration, 30 mm/s, carbon steel
| Power | Penetration | mm per kW | Note |
|---|---|---|---|
| 1 kW | 1.1 mm | 1.10 | Conduction to keyhole transition |
| 2 kW | 2.3 mm | 1.15 | Stable keyhole |
| 3 kW | 3.2 mm | 1.07 | Sweet spot for 3 mm |
| 4 kW | 4.1 mm | 1.03 | — |
| 6 kW | 5.8 mm | 0.97 | Needs helium mix |
| 8 kW | 7.0 mm | 0.88 | Diminishing |
| 12 kW | 9.5 mm | 0.79 | Wobble or twin-spot helps |
3. Three conditions that decide whether you get the rule
Speed. The rule is only valid at the speed where the keyhole is stable. Halve the speed and penetration rises 40%, not 100%. Double it and penetration collapses because the keyhole never opens.
Focus. Zero focus is wrong for deep penetration. Setting focus 2–3 mm below the surface uses the converging beam to preheat and increases penetration 15% at the same power.
Gas. Argon caps penetration. Helium or a helium mix is required above 6 kW, because helium’s higher ionisation energy suppresses the plasma that blocks the beam.
4. What breaks the rule
Poor beam quality. An M² of 4 spreads energy over a 200 µm spot; the same watts give 30% less depth.
Thick oxide or mill scale. Absorbs energy at the surface and shifts the keyhole start point.
Gap between sheets. A 0.1 mm gap costs 0.4 mm of penetration — the beam has to close the gap first.
Frequently asked questions
Does the rule work for stainless?
Roughly 0.8 mm/kW, because stainless conducts less heat away but also absorbs at a different rate. Budget 20% more power than carbon steel for the same depth.
Can I get 10 mm with 10 kW?
On carbon steel with helium and a 200 mm lens, sometimes — at 8 mm/s. It is technically inside the machine’s envelope and economically outside anyone’s production plan.
Why does penetration drop when I increase speed slightly?
Because keyhole stability has a threshold, not a slope. Just past the limit the keyhole collapses intermittently and the weld becomes a series of conduction-mode pockets.