Quick answer: for a 1–3 mm stainless weld with a 10 mm nozzle, 15–20 L/min is the window. Under 10 L/min you get oxidation and a grey bead; over 35 L/min the gas jet becomes turbulent at the nozzle exit, drags air into the plume and creates porosity — the exact defect the gas was supposed to prevent. Gas flow has an optimum, and it is narrower than most operators assume.
1. Flow rate by nozzle diameter
| Nozzle bore | Minimum flow | Optimum | Upper limit | Typical use |
|---|---|---|---|---|
| 6 mm | 6 L/min | 8–12 L/min | 15 L/min | Thin sheet, high speed |
| 8 mm | 8 L/min | 12–16 L/min | 20 L/min | General welding |
| 10 mm | 10 L/min | 15–20 L/min | 25 L/min | 1–3 mm stainless |
| 12 mm | 12 L/min | 18–24 L/min | 30 L/min | Thicker section, wobble |
| 16 mm | 15 L/min | 22–30 L/min | 36 L/min | Deep penetration, aluminium |
The upper limit rises roughly with bore squared, because the turbulent transition happens at a fixed exit velocity. That is why “turn the gas up” works on a big nozzle and fails on a small one.
2. Why too much gas causes porosity
Above the critical exit velocity the jet loses laminar structure and entrains ambient air at its boundary. Air contains nitrogen and moisture; both dissociate in the keyhole and the nitrogen recombines as bubbles when the melt solidifies. The result is a bead that looks clean from outside with porosity visible only on a cross-section — the worst kind of defect because it passes visual inspection.
The tell-tale is that porosity gets worse as you increase flow. If doubling the gas makes it worse, stop increasing it.
3. Gas selection changes the flow rate
| Gas | Flow multiplier | Effect |
|---|---|---|
| Argon | 1.0× | Baseline, calm arc-free plume |
| Nitrogen | 0.9× | Faster, slight nitro-carburising on steel |
| Helium | 1.4× | Higher ionisation energy, better keyhole stability at speed |
| Ar + 2% O₂ | 1.0× | Improves wetting on carbon steel only |
| Ar + 30% He | 1.2× | Balance of cost and keyhole stability |
Helium needs more flow because it is lighter and diffuses out of the plume faster — but it also tolerates higher flow before turbulence, so the usable window is wider even though the numbers are higher.
4. Three checks that find the real problem
Nozzle stand-off. Doubling the distance from 5 mm to 10 mm halves the effective shielding. Check stand-off before touching flow.
Leaks downstream of the solenoid. A loose push-fit connector bleeds 2–3 L/min and the flowmeter still reads the setpoint.
Cross-draught. An open workshop door 3 m away is enough. Weld a test coupon with the door closed and compare.
Frequently asked questions
Is pre-flow necessary for laser welding?
Yes, 0.3–0.5 s. Laser welding starts in milliseconds, so the gas must already be in place. Without pre-flow the first 2 mm of every weld is oxidised — which is often where a leak path forms.
Does a trailing shield help?
On stainless above 2 mm, yes. The main nozzle shields the keyhole; a trailing shield keeps oxygen off the cooling bead. It adds roughly 8 L/min and eliminates the heat tint without lowering the main flow.
Why does aluminium need more flow than steel?
Aluminium conducts heat away five times faster, so the melt pool is wider and the plume larger. The gas has to cover a bigger area at the same velocity, and helium is often used — both push the flow up.
Related reading
Intouchray has manufactured industrial fibre laser cutting, welding, cleaning and cladding machines in Dongguan, Guangdong, China since 2001, with additional bases in Wuhan and Korea. Minimum order is one machine, built to order.