Quick answer: kerf width is 0.12–0.2 mm on 1 mm sheet, 0.2–0.3 mm at 3 mm and 0.4–0.6 mm at 10 mm. A 0.1 mm tolerance is achievable, but only if you control focus position, nozzle wear, gas pressure and speed — in that order of influence. Nesting software that assumes a fixed kerf is the most common reason parts come out undersize.
1. Typical kerf by thickness
| Thickness | Nitrogen kerf | Oxygen kerf | Dominant variable |
|---|---|---|---|
| 1 mm | 0.12–0.15 mm | 0.15–0.20 mm | Focus position |
| 2 mm | 0.15–0.20 mm | 0.20–0.25 mm | Focus position |
| 3 mm | 0.20–0.28 mm | 0.25–0.32 mm | Gas pressure |
| 6 mm | 0.30–0.40 mm | 0.35–0.45 mm | Gas pressure |
| 10 mm | 0.40–0.55 mm | 0.45–0.60 mm | Nozzle bore |
2. The six variables, ranked by influence
| Variable | Kerf change | How to control it |
|---|---|---|
| Focus position | ±0.04 mm per 0.5 mm defocus | Fixed focus-height sensor, weekly calibration |
| Nozzle wear | +0.03 mm after 2000 pierces | Replace on a count, not on appearance |
| Gas pressure | +0.05 mm at +20% pressure | Regulator with 0.1 bar resolution |
| Cut speed | +0.02 mm at −15% speed | Lock speed, adjust power instead |
| Material batch | ±0.02 mm | First-article check per coil |
| Machine acceleration | +0.03 mm on tight corners | Corner rounding in the CAM, not the machine |
Two variables account for 70% of the drift: focus and nozzle. Both are consumable-driven, which is why a kerf that was perfect in March is 0.03 mm wide in June without anyone touching a setting.
3. Holding 0.1 mm on a real part
Measure the first part of every shift on the same feature and log it. Kerf drifts slowly and then fails an inspection all at once.
Compensate in CAM with the measured kerf of that material and thickness, not with the machine’s default table.
Keep a separate compensation value per gas. Nitrogen and oxygen kerfs differ by 0.05 mm on the same thickness.
Never adjust focus to fix a dimension problem — adjust the CAM. Focus moves the kerf on both sides of the cut and the compensation stops being valid.
Frequently asked questions
Why is the kerf wider at the bottom than the top?
Gas erosion. Above the optimum pressure the jet keeps removing material after the beam has passed. Reduce pressure 1 bar, or move the focus down 0.5 mm and re-test.
Does a smaller nozzle give a smaller kerf?
Only up to a point. Below about 1.2 mm bore the jet becomes unstable and the kerf widens again with dross. Match the bore to the thickness, not to the tolerance target.
How often should the nozzle be replaced?
On a pierce count. For 3 mm stainless, roughly every 1500–2000 pierces. A nozzle that looks clean can still be 0.03 mm out of round, and that is 30% of your tolerance budget.