# Galvanized Steel Laser Welding: Controlling Zinc Porosity

[Home](https://www.intouchray.com) - [Technical Support](https://www.intouchray.com/category/technical-support/) - Galvanized Steel Laser Welding: Controlling Zinc Porosity

**Quick answer:** zinc boils at 907 °C while steel melts at 1450 °C. The coating vaporises before the weld pool even forms, and the vapour has nowhere to go but up through the melt — which is why galvanized laser welds are porous. Three things fix it: a 0.1–0.15 mm gap between sheets, pulse modulation at 200–500 Hz, and speed high enough that the vapour escapes before the pool closes.

## 1. Why galvanized is different

A Z275 coating is 20 µm per side, which is roughly 0.14 kg/m² of zinc. When the beam reaches it, the zinc vaporises instantly and expands about 900 times in volume. In a closed lap joint that vapour pressure pushes through the only available path: the melt pool. The result is a wormhole, not a round pore.

## 2. Porosity by parameter set

| Setup | Porosity (area %) | Comment |
| ----- | ----------------- | ------- |
| Zero gap, CW, 30 mm/s | 18% | Unusable |
| Zero gap, 300 Hz modulation | 9% | Better, still fails pressure test |
| 0.1 mm gap, CW | 6% | Vapour escapes through the gap |
| 0.1 mm gap, 300 Hz modulation | 2% | Production-usable |
| 0.15 mm gap, 300 Hz, 50 mm/s | 1.5% | Gap must be controlled by fixture |

The gap is not a workaround for poor fit-up — it is a designed vent. Fixtures for galvanized work should hold 0.1 mm, not clamp to zero.

## 3. The three levers, in order

- **Gap.** Biggest effect, cheapest change. Add a 0.1 mm shim to the fixture and porosity halves.

- **Modulation.** Pulsing gives the vapour a window to escape between pulses. 200–500 Hz at 60–80% duty is the useful range.

- **Speed.** Faster welds have a shorter pool and a shorter escape path. Going from 25 to 50 mm/s often removes more porosity than any other change.

Do not increase power to "burn through" the zinc. Higher power vaporises more zinc and deepens the keyhole, which makes the escape path longer. Porosity gets worse.

## Frequently asked questions

### Can I weld galvanized steel without removing the coating?

Yes, with a gap and modulation, and if the joint is not required to be airtight. For pressure-tight joints, strip 5 mm of coating from the weld zone.

### Does this also apply to galvanealed and zinc-aluminium coatings?

Galvanealed is easier because the coating is already alloyed and less volatile. Zinc-aluminium (ZnAl) is worse than pure zinc because aluminium raises the vapour pressure. Budget 30% more porosity than the table above.

### What about weld strength?

Porosity below 3% has little effect on static strength, but it ruins fatigue life and any leak specification. For structural galvanized parts, specify 2% maximum and verify by cross-section, not by visual inspection.

## Related reading

- [Shielding gas flow rate and porosity](https://www.intouchray.com/laser-welding-shielding-gas-flow-rate-lpm-porosity/)

- [Wobble welding and gap bridging](https://www.intouchray.com/wobble-welding-amplitude-frequency-gap-bridging/)