title: "Penetration Depth per kW: Testing the 1 mm/kW Rule"
url: https://www.intouchray.com/laser-welding-penetration-depth-mm-per-kw/
date: 2026-11-10
modified: 2026-11-10
lang: en
author: "Sales11@taiyilaser.com"
description: "Quick answer: on carbon steel at 30 mm/s, penetration runs close to 1 mm per kW from 1 kW to 6 kW. Above 6 kW the curve flattens because plasma..."
categories:
  - "Technical Support"
word_count: 380
---

# Penetration Depth per kW: Testing the 1 mm/kW Rule

[Home](https://www.intouchray.com) - [Technical Support](https://www.intouchray.com/category/technical-support/) - Penetration Depth per kW: Testing the 1 mm/kW Rule

**Quick answer:** on carbon steel at 30 mm/s, penetration runs close to 1 mm per kW from 1 kW to 6 kW. Above 6 kW the curve flattens because plasma absorption in the keyhole caps how much energy reaches the bottom. If you need 10 mm, plan for 12 kW plus helium, not 10 kW.

## 2. Measured penetration, 30 mm/s, carbon steel

| Power | Penetration | mm per kW | Note |
| ----- | ----------- | --------- | ---- |
| 1 kW | 1.1 mm | 1.10 | Conduction to keyhole transition |
| 2 kW | 2.3 mm | 1.15 | Stable keyhole |
| 3 kW | 3.2 mm | 1.07 | Sweet spot for 3 mm |
| 4 kW | 4.1 mm | 1.03 | — |
| 6 kW | 5.8 mm | 0.97 | Needs helium mix |
| 8 kW | 7.0 mm | 0.88 | Diminishing |
| 12 kW | 9.5 mm | 0.79 | Wobble or twin-spot helps |

## 3. Three conditions that decide whether you get the rule

**Speed.** The rule is only valid at the speed where the keyhole is stable. Halve the speed and penetration rises 40%, not 100%. Double it and penetration collapses because the keyhole never opens.

**Focus.** Zero focus is wrong for deep penetration. Setting focus 2–3 mm below the surface uses the converging beam to preheat and increases penetration 15% at the same power.

**Gas.** Argon caps penetration. Helium or a helium mix is required above 6 kW, because helium's higher ionisation energy suppresses the plasma that blocks the beam.

## 4. What breaks the rule

- **Poor beam quality.** An M² of 4 spreads energy over a 200 µm spot; the same watts give 30% less depth.

- **Thick oxide or mill scale.** Absorbs energy at the surface and shifts the keyhole start point.

- **Gap between sheets.** A 0.1 mm gap costs 0.4 mm of penetration — the beam has to close the gap first.

## Frequently asked questions

### Does the rule work for stainless?

Roughly 0.8 mm/kW, because stainless conducts less heat away but also absorbs at a different rate. Budget 20% more power than carbon steel for the same depth.

### Can I get 10 mm with 10 kW?

On carbon steel with helium and a 200 mm lens, sometimes — at 8 mm/s. It is technically inside the machine's envelope and economically outside anyone's production plan.

### Why does penetration drop when I increase speed slightly?

Because keyhole stability has a threshold, not a slope. Just past the limit the keyhole collapses intermittently and the weld becomes a series of conduction-mode pockets.

## Related reading

- [Laser welding heat input in J/mm](https://www.intouchray.com/laser-welding-heat-input-j-per-mm-calculation/)

- [Keyhole vs conduction welding](https://www.intouchray.com/key-hole-vs-heat-conduction-welding-15mm-threshold-defined/)