title: "Assist Gas Pressure by Thickness: Nitrogen vs Oxygen"
url: https://www.intouchray.com/laser-cutting-assist-gas-pressure-bar-by-thickness/
date: 2026-11-10
modified: 2026-11-10
lang: en
author: "Sales11@taiyilaser.com"
description: "Quick answer: nitrogen is a high-pressure gas (12–22 bar) because it only has to push molten metal out; oxygen is a low-pressure gas (0.5–2 bar) because it also has to..."
categories:
  - "Technical Support"
word_count: 535
---

# Assist Gas Pressure by Thickness: Nitrogen vs Oxygen

[Home](https://www.intouchray.com) - [Technical Support](https://www.intouchray.com/category/technical-support/) - Assist Gas Pressure by Thickness: Nitrogen vs Oxygen

**Quick answer:** nitrogen is a high-pressure gas (12–22 bar) because it only has to push molten metal out; oxygen is a low-pressure gas (0.5–2 bar) because it also has to burn. Setting 15 bar on carbon steel with oxygen does not cut faster — it destroys the edge and doubles gas cost. Pressure is a function of thickness and gas type, never of "more is better".

## 1. Nitrogen pressure by thickness

| Thickness (stainless) | Nozzle pressure | Nozzle bore | Stand-off |
| --------------------- | --------------- | ----------- | --------- |
| 1 mm | 10–12 bar | 1.2 mm | 0.8 mm |
| 2 mm | 12–14 bar | 1.4 mm | 0.8 mm |
| 3 mm | 14–16 bar | 1.6 mm | 1.0 mm |
| 6 mm | 16–18 bar | 2.0 mm | 1.2 mm |
| 10 mm | 18–20 bar | 2.5 mm | 1.5 mm |
| 15 mm | 20–22 bar | 3.0 mm | 2.0 mm |

Nozzle bore and stand-off rise with pressure because a small bore cannot deliver 20 bar without excessive velocity loss, and a short stand-off puts the shock wave inside the kerf.

## 2. Oxygen pressure by thickness

| Thickness (carbon steel) | Nozzle pressure | Nozzle bore | Cut speed (3 kW) |
| ------------------------ | --------------- | ----------- | ---------------- |
| 1 mm | 0.5–0.8 bar | 1.0 mm | 8.0 m/min |
| 3 mm | 0.8–1.0 bar | 1.2 mm | 4.5 m/min |
| 6 mm | 1.0–1.4 bar | 1.4 mm | 2.6 m/min |
| 10 mm | 1.2–1.8 bar | 1.6 mm | 1.6 m/min |
| 16 mm | 1.5–2.0 bar | 2.0 mm | 0.9 m/min |

Above roughly 2.5 bar on oxygen the reaction becomes uncontrolled: the kerf widens, the edge glows, and dross sticks. If you need more than 2.5 bar to get through a thickness, the answer is more power, not more gas.

## 3. Reading wrong pressure from the cut

| Symptom | Cause | Fix |
| ------- | ----- | --- |
| Hard dross, weldable, on the bottom edge | Nitrogen pressure too low | +2 bar, then re-check focus |
| Soft dross that wipes off | Speed too high, not pressure | Reduce speed 10% first |
| Kerf wider at the bottom than the top | Pressure too high, gas erodes the kerf | −2 bar or a larger bore |
| Striations leaning backwards | Oxygen pressure too low for the speed | +0.2 bar in 0.2 bar steps |
| Random missed cuts on thin sheet | Pressure too high lifts the sheet | Drop to 6–8 bar, add micro-joints |

## 4. The cost nobody budgets

Nitrogen at 18 bar through a 2.5 mm nozzle consumes roughly 45 Nm³/h. At typical industrial liquid nitrogen pricing that is the single largest consumable cost on a fiber laser — larger than electricity for stainless work. Dropping from 20 bar to 16 bar where the thickness allows cuts gas consumption by about 18% with no speed penalty.

This is why gas-pressure optimisation is usually the fastest payback project on an existing machine: it needs a flow meter and a day of trials, not capital.

## Frequently asked questions

### Can I cut stainless with compressed air to save nitrogen?

Yes, up to about 3 mm, if the oxide edge is acceptable. Air cutting leaves a grey oxidised edge that must be pickled or brushed. For visible stainless parts it is not an option.

### Why does pressure drop when the nozzle gets dirty?

Because the gauge reads supply pressure, not nozzle pressure. Spatter on the nozzle face throttles the exit and the cut quality falls while the gauge still shows 18 bar. Check the nozzle every 4 hours on thick-section work.

### Is higher purity nitrogen worth it?

For 3 mm and above, yes. 99.999% versus 99.99% changes the edge from light yellow to bright silver on stainless. Below 2 mm the difference is hard to see and the cost difference is not justified.

## Related reading

- [Fiber laser cutting thickness chart](https://www.intouchray.com/fiber-laser-cutting-thickness-power-chart-1kw-30kw/)

- [Kerf width and 0.1 mm tolerance](https://www.intouchray.com/laser-cutting-kerf-width-tolerance-parameters/)