title: "Laser Welding Heat Input: J/mm Calculation and Distortion Control"
url: https://www.intouchray.com/laser-welding-heat-input-j-per-mm-calculation/
date: 2026-11-10
modified: 2026-11-10
lang: en
author: "Sales11@taiyilaser.com"
description: "Quick answer: laser welding heat input is Q = P / v, where P is laser power in watts and v is welding speed in mm/s. The result is expressed..."
categories:
  - "Technical Support"
word_count: 771
---

# Laser Welding Heat Input: J/mm Calculation and Distortion Control

[Home](https://www.intouchray.com) - [Technical Support](https://www.intouchray.com/category/technical-support/) - Laser Welding Heat Input: J/mm Calculation and Distortion Control

**Quick answer:** laser welding heat input is **Q = P / v**, where P is laser power in watts and v is welding speed in mm/s. The result is expressed in J/mm. For 0.5–3 mm stainless and carbon steel, a well-tuned fiber laser weld sits between **8 and 45 J/mm** — roughly one tenth of an equivalent TIG weld. Below 6 J/mm you get lack of fusion; above 80 J/mm thin sheet starts to bow.

## 1. The formula and what each term actually means

Q (J/mm) = P (W) ÷ v (mm/s). Power is measured at the workpiece, not at the source: a 2 kW source with 88% delivery efficiency puts 1,760 W into the part. Speed is the actual travel speed of the stage or robot, not the commanded feed rate. When either number is wrong by 10%, heat input is wrong by 10% — and so is your weld bead width.

Because the relationship is inverse, doubling speed halves heat input but also halves penetration depth. That single trade-off is why heat input charts and penetration charts are the same chart read in two directions.

## 2. Measured heat input by thickness

| Material | Thickness | Power (W) | Speed (mm/s) | Heat input (J/mm) | Typical result |
| -------- | --------- | --------- | ------------ | ----------------- | -------------- |
| 304 stainless | 0.5 mm | 500 | 60 | 8.3 | Conduction mode, no discolouration |
| 304 stainless | 1.0 mm | 1,000 | 50 | 20 | Full penetration, 0.9 mm bead |
| 304 stainless | 2.0 mm | 2,000 | 45 | 44 | Keyhole start, slight undercut |
| Q235 carbon steel | 3.0 mm | 3,000 | 40 | 75 | Keyhole, 3.0 mm penetration |
| Q235 carbon steel | 6.0 mm | 6,000 | 30 | 200 | Deep keyhole, needs fixture clamping |

Read the first column down and the pattern is obvious: every doubling of thickness costs a little more than double the heat input, because conduction losses grow with the thermal mass behind the weld.

## 3. Why J/mm matters more than watts

Two machines can both claim "2 kW" and produce completely different parts. At 20 mm/s the 2 kW machine delivers 100 J/mm and bows a 1 mm panel. At 80 mm/s the same machine delivers 25 J/mm and leaves the panel flat. Buyers who compare kilowatts are comparing the wrong number.

Heat input also drives three downstream costs: post-weld straightening, heat tint removal, and fixture wear. A 30% reduction in J/mm typically removes one straightening operation from a 1.5 mm stainless assembly.

## 4. Reading the defects back to the number

| Symptom | Heat input | First parameter to change |
| ------- | ---------- | ------------------------- |
| Lack of fusion at the root | Too low (< 6 J/mm) | Reduce speed 15%, keep power |
| Spatter on the top bead | Too high at the surface | Defocus +1 mm, raise speed |
| Undercut on both sides | Too high | Lower power 10%, add wobble |
| Blow-through on thin sheet | Far too high | Switch to pulsed mode, 30% duty |
| Grey/blue oxidation halo | Marginal | Increase shielding gas, not power |

## 5. How to hold heat input constant across a batch

- Log P and v per part, not per shift. Drift hides in averages.

- Measure power at the workpiece with a calorimeter once a month; delivery fibre degradation shows up as falling Q long before it shows as a bad weld.

- Lock speed in the program and adjust power only — operators can feel a speed change, they cannot feel a 3% power change.

- Keep a J/mm window per part number in the work instruction, the same way you keep a torque spec.

## Frequently asked questions

### Is laser welding heat input the same as arc welding heat input?

The formula is identical, Q = P/v, but the efficiency term differs. Arc processes lose 20–40% of the input to the arc and spatter; fiber laser delivery loses 8–15%. That is why a 20 J/mm laser weld and a 20 J/mm TIG weld do not produce the same heat-affected zone — the laser puts more of its energy where you aimed it.

### What heat input do I need for 1 mm stainless?

18–25 J/mm for full penetration without distortion. On a 1 kW source that is 40–55 mm/s. Go below 15 J/mm and the root becomes intermittent; above 30 J/mm the part needs clamping or a copper backing bar.

### Does wobble welding change the calculation?

Yes. Wobble spreads the same energy over a wider track, so effective heat input per unit area drops while Q per unit length stays the same. Use Q for distortion prediction and energy density (W/cm²) for penetration prediction — they move in opposite directions when you change amplitude.

### Can I exceed 200 J/mm on thick plate?

You can, and on 8 mm and above you often must. The limit is not the number itself but the fixture: above roughly 150 J/mm, thermal expansion during the pass exceeds what a standard clamp can hold, and the part moves while it is being welded.

## Related reading

- [Focal position and spot size optimization](https://www.intouchray.com/laser-focal-position-spot-size-optimization/)

- [Laser beam quality and the M² factor](https://www.intouchray.com/laser-beam-quality-m2-factor-guide/)

- [Keyhole vs conduction welding: the 1.5 mm threshold](https://www.intouchray.com/key-hole-vs-heat-conduction-welding-15mm-threshold-defined/)